Geometry and Fit Specifications

  • Positive Draft Angles: All vertical pocket walls, outer tray skirts, and internal dividers slope inward from the top flange to the pocket floor. Deeper wells and textured mold surfaces require steeper draft than shallow, smooth-walled cavities so the cooled plastic releases without dragging or scuffing.
  • Pocket Corner Radii: Both horizontal plan-view corners and vertical wall-to-floor and wall-to-flange intersections use continuous rounded fillets. Smooth transitions prevent localized stretching at the pocket base and eliminate sharp troughs where heated sheet bridges across adjacent wells.
  • Fluted Stiffening Ribs: Vertical flutes pressed into outer perimeter walls and long divider walls, combined with stepped or recessed channels across wide pocket floors, increase rigidity through cross-sectional geometry. Ribs prevent thin-gauge trays from bowing inward under lid pressure or sagging when lifted loaded.
  • Floor-Level Clearance and Card Fit: Because positive draft narrows each pocket toward its base, internal well dimensions must be checked at the pocket floor rather than at the top rim: Floor Clearance = Top Pocket Width - (2 * Well Depth * tan(Draft Angle)) - Component Width For card wells, floor clearance and corner fillets must accommodate the deck's actual trimmed footprint, corner rounding (such as R3–R3.5 mm / 0.118–0.138 in), and total stack height—accounting for card caliper (0.28–0.31 mm / 0.011–0.012 in for 300 gsm art/blue core up to 0.40–0.44 mm / 0.016–0.017 in for 400 gsm, plus 0.03–0.05 mm / 0.001–0.002 in per card with double-sided film).
  • Box Fit Tolerances: Outer tray dimensions and loaded height must sit within standard box clearances of 1.5–2.5 mm (0.059–0.098 in) across width and height and 1.5–3 mm (0.059–0.118 in) for stack height.

Production Steps

  1. Tooling CAD and Relief Modeling: Apply positive draft to every vertical wall, add continuous corner and base fillets, and place stiffening flutes along unsupported outer walls and long divider spans. Confirm component and tooling minimums for the boxed game before cutting the mold.
  2. Mold Machining and Venting: Machine the forming tool with smooth surface transitions and drill vacuum bleed holes in deep pocket corners, rib roots, and narrow divider troughs so trapped air escapes during draw.
  3. Sheet Heating and Vacuum Forming: Heat the plastic sheet evenly to its forming window, draw it onto the mold under vacuum until all ribs and corner fillets are fully defined, and hold cooling until the part stabilizes below distortion temperature before ejection.
  4. Flange Trimming and De-Nesting Check: Trim the outer flange to the target box footprint and stack-test nested trays to confirm they separate cleanly without locking along the drafted walls.

Sign-Off Criteria

  • Mold Release and De-Nesting: Trays eject cleanly with no drag marks, tearing, or stress-whitening along vertical walls, and nested stacks separate without jamming.
  • Uniform Wall Distribution: Pocket corners and rib peaks show consistent opacity and thickness with no pinholes, splits, or brittle thin spots.
  • Component Seating: Decks and game pieces drop flat onto the pocket floor without pinching against the tapered lower walls or snagging on corner fillets.
  • Structural Rigidity and Box Fit: Loaded trays fit within the 1.5–2.5 mm (0.059–0.098 in) width/height and 1.5–3 mm (0.059–0.118 in) stack-height box clearances, and outer ribbed walls remain upright without buckling when lifted.

Concrete Failure Modes

  • Sheet Webbing (Bridging): Insufficient divider width between deep pockets, tight divider radii, or blocked vacuum vents cause the heated sheet to stretch across the gap between adjacent cavities instead of forming down to the mold floor.
  • Wall Buckling and Oil-Canning: Tall, unribbed outer skirts or wide flat tray floors flex inward under box lid compression or bow downward under heavy card stacks.
  • Corner Thinning and Cracking: Sharp vertical or base corner radii in deep-draw pockets over-stretch the sheet at the bottom corners, producing fragile spots that crack during transit or de-nesting.
  • Mold Lock and Card Pinching: Zero or negative draft angles lock the cooled plastic onto the tool, while steep draft without compensating top-rim width narrows the pocket floor and causes lower cards in a deck to bind or curl.