Inspecting a defective pad follows a fixed order: first check the glued top edge for ink or coating contamination, next inspect the padding compound film for under- or over-penetration, and finally verify that the chipboard backer is present and jogged flush to the spine. For related binding and paper-extra issues, see booklets and printed paper troubleshooting.
Ordered Diagnostic Checks
1. Check the Top Edge for Ink, Varnish, or Coating
Look at the detached sheet's top edge under angled light. If the edge is glossy, slick, or solid-inked and the glue peels off cleanly in a strip without pulling paper fibers, surface contamination blocked adhesion.
- Competing cause ruled out: If paper fibers are torn off onto the glue strip, the glue bonded to the sheet and the failure lies in compound penetration or stock weight rather than surface blocking.
2. Check Padding-Compound Penetration and Film Flexibility
Inspect the spine of the pad and the top edge of both loose and remaining sheets:
- Sheets falling out in clumps or individually without resistance: The padding compound bridged the outside edge without wicking into the paper fibers, or the compound dried too brittle and cracked when flexed.
- Sheets ripping raggedly into the score grid: The compound was too thin or applied too heavily, wicking down between individual sheets and welding them together below the trim line.
3. Check Chipboard Backing Support and Alignment
Check the back of the pad. A missing, undersized, or recessed chipboard backer removes the rigid leverage needed to tear a single sheet cleanly against the spine. If the backer is present but detached, the board was either recessed behind the paper stack during jogging or oriented with a slick coated face toward the spine.
Relevant Specifications
| Parameter | Specification | Notes |
|---|---|---|
| Sheet stock | 80–120 gsm (about 0.08–0.13 mm / 0.003–0.005 in per sheet) | Uncoated offset text stock absorbs padding compound evenly and tears cleanly. |
| US basis weight distinction | US Text LB (25 x 38 in / 635 x 965 mm) vs. Cover LB (20 x 26 in / 508 x 660 mm) | 80–120 gsm aligns with roughly 55–80 lb Text; specifying Cover LB by mistake produces stiff sheets that resist clean top-edge tearing. |
| Backing board | 1.5–2 mm (0.059–0.079 in) greyboard / chipboard | Provides rigid spine support during tearing and transit. |
| Bleed and safety | 3 mm (0.118 in) bleed per side; >=3 mm (0.118 in) safety | Keep score grids and critical text >=3 mm (0.118 in) from the glued top edge. |
| Ink and color limits | CMYK with separate spot layers, >=300 DPI, TAC <=280%–300% | Heavy ink coverage at the bleed edge reduces fiber absorbency; keep varnish or aqueous coating off the glue edge. |
For custom scorepad dimensions, choose trim sizes that fit the box or game insert layout without forcing awkward sheet proportions that twist when torn.
Job-Specific Production Steps and Sign-Off Criteria
Card Deck Press produces scorepads through specialist offset and tabletop manufacturing partners using the following sequence:
- Prepress and coating knockout: Prepare press-ready PDF/X-1a or PDF/X-4 files with outlined or embedded fonts. Keep flood varnishes, UV coatings, and dense rich black (C40–60 M30–40 Y30–40 K100) clear of the binding edge so raw paper fibers remain exposed at the cut line.
- Jogging and clamping: Jog the printed sheets and the chipboard backer together so the top binding edge is completely flush. Clamp the stack under uniform pressure so compound cannot seep between sheets.
- Padding-compound application: Apply flexible PVA-based padding compound in controlled, thin coats along the clamped spine. Allow full cure before releasing clamp pressure or handling stacks.
- Final trim and carton packing: Trim the remaining edges cleanly if trimmed post-padding, and pack pads flat in shipping cartons—typically 10–15 kg (22–33 lb) per carton—so stacks do not bow or shear along the glue spine in transit.
Sign-Off Criteria
- Holding a pad upside down by the bottom corners and shaking lightly keeps all sheets attached to the spine.
- Pulling a single top sheet at a 45-degree angle detaches it cleanly along the top edge without tearing into the printed area or loosening the sheet underneath.
- The chipboard backer stays bonded to the final sheet and the spine film across the full pad width.
Concrete Failure Modes
| Symptom | Physical Cause | Prevention / Correction |
|---|---|---|
| Sheets drop out in blocks or clean strips | Top-edge varnish, aqueous coating, or heavy ink blocked glue penetration; or sheets were not jogged flush before gluing. | Knock out coatings from the binding edge; jog sheets and backers flush before clamping. |
| Sheets tear raggedly down into the grid | Low-viscosity compound wicked between loosely clamped sheets, or stock is too heavy/coated to tear cleanly along the glue line. | Use 80–120 gsm (0.08–0.13 mm / 0.003–0.005 in) uncoated text stock; clamp firmly and apply thin coats. |
| Chipboard backer separates from the pad | Backer sat slightly recessed from the spine during jogging, or a coated board face was placed against the glue. | Jog the 1.5–2 mm (0.059–0.079 in) backer flush with the sheets and orient the raw board edge to the spine. |
| Pads curl and pop loose after shipping | Missing backing board or uneven stacking under 10–15 kg (22–33 lb) carton loads flexed the cured glue film. | Always include a rigid chipboard backer and pack scorepads flat without unsupported overhang. |
Parent guide Rulebook and Play Aid Troubleshooting
Related guides
- Why Does Lamination Bubble or Lift on Rulebook Covers and Reference Sheets?
- Why Are Staples Loose, Crooked, or Tearing Through Saddle-Stitched Booklets?
- Why Do Rulebook Pages Ripple or Covers and Reference Sheets Curl?
- Why Are Pages Out of Order, Missing, or Duplicated in a Bound Rulebook?
- Why Do Wire-O Bound Reference Guides Arrive Crushed or Snag Pages?
- Why Do Clue Envelope Seams Pop Open or Flaps Fail to Seal?