Choose hot-knife (thermal) welding for standard cast polypropylene (CPP) sleeves where a broader melt window produces a smooth, ductile side bead, and choose ultrasonic welding for oriented polypropylene (OPP/BOPP), multi-layer matte-textured films, or high-speed runs where localized frictional heating avoids warping the surrounding film. For broader sleeve geometry, opening styles, and top-or-bottom seal layouts, see Card Sleeve Welding and Openings.
Specifications and Welding Conditions
| Parameter | Hot-Knife (Thermal) Welding | Ultrasonic Welding |
|---|---|---|
| Best-fit sleeve film | Mono-layer CPP and thicker PP gauges | Oriented PP (OPP/BOPP), matte-coated, or multi-layer films |
| Typical weld seam width | 0.8–1.5 mm (0.031–0.059 in) | 0.5–1.2 mm (0.020–0.047 in) |
| Heat mechanism | Conductive transfer from heated blade/jaw | High-frequency mechanical vibration at the ply interface |
| Key control variables | Blade temperature, dwell time, clamping pressure | Horn amplitude, weld time, trigger force, hold time |
| Heat-affected zone (HAZ) | Wider; requires controlled cooling under pressure | Narrow; minimal thermal spread into the card pocket |
- Film orientation and coating: CPP melts evenly under conductive heat without severe shrinkage, making hot-knife blades reliable. Oriented PP (OPP/BOPP) and matte-textured outer coatings resist conductive heat transfer and shrink if overheated; ultrasonic energy focuses heat directly at the inner interface so the outer surface stays flat.
- Seam width vs. pocket clearance: A wider weld bead (1.0–1.5 mm / 0.039–0.059 in) resists peel forces better if the polymer is fully fused, but it adds to the outer sleeve width and tightens box fit. Keep side seams consistent so cards slide in without binding against the weld edge and sleeved decks still fit their target box clearance.
- Dwell and hold consistency: Both methods require stable clamping force during the cooling or hold phase immediately after energy input. Releasing pressure while the PP or CPP interface is still molten causes the plies to spring apart and weakens the mouth corners.
Production Steps
- Web tensioning and ply registration: Feed the front and back PP or CPP plies under balanced tension so both layers lie flat across the weld zone without curl, wrinkles, or trapped air pockets.
- Tooling calibration: Set hot-knife blade temperature and dwell duration—or ultrasonic horn amplitude, weld time, and anvil parallelism—to match the film gauge and surface finish (gloss vs. matte).
- Side-seam welding and hold: Actuate the weld along both side edges from the closed bottom fold/seal up to the open mouth, maintaining clamping pressure through the hold window until the fused polymer solidifies.
- Synchronized trimming and separation: Cut or slit along the outer edge of the weld line without nicking the fused bead, leaving a clean termination right at the sleeve mouth.
Sign-Off Criteria
- Continuous weld bead: The seam shows uniform translucency or fusion texture from bottom to mouth with no unsealed skips, pinholes, or charred spots.
- Clean mouth-corner termination: Both top corners end flush with the mouth cut, free of jagged nicks, loose film tails, or delaminating "ears" that catch during mash shuffling.
- Peel-strength behavior: Pulling the front and back plies apart at the mouth corners causes the adjacent film to stretch or yield before the weld line separates, rather than zipping open cleanly along the interface.
- Flatness and dimensional stability: Side edges remain straight without thermal puckering or wavy distortion that increases stack thickness or catches card corners on insertion.
Concrete Failure Modes
- Mouth-corner unzipping: Insufficient dwell time, low ultrasonic amplitude, or matte/slip additives in the weld zone prevent complete molecular fusion. The seam holds during light handling but splits downward from the mouth corners when cards wedge between plies during mash shuffling.
- Heat-affected zone (HAZ) embrittlement: Excessive hot-knife temperature or overly long dwell degrades PP/CPP polymer chains right beside the weld bead. The seam appears fused on inspection, then cracks brittlely along the edge of the bead under riffle flexing.
- Burn-through and pinholes: Uneven anvil pressure, carbon buildup on a hot knife, or ultrasonic energy spikes melt through thin spots in the film, leaving holes or sharp burrs that snag card corners.
- Thermal puckering and wavy edges: Unbalanced web tension or premature release of hold pressure before the weld cools causes the seam to contract unevenly, creating rippled edges that catch during shuffling and inflate deck height.
- Slitting nicks along the seam: Lateral drift between the weld station and the side-trimming blade cuts into the fused bead, creating a stress-concentration notch that initiates tears at the mouth.
Parent guide Card Sleeve Welding and Opening Construction