Paperboard Grades, Caliper, and Basis Weight
Postcard stock stiffness scales with board caliper rather than weight alone. US paper weights distinguish Cover LB (20 × 26 in basis sheet) from Text LB (25 × 38 in basis sheet); a 300 gsm board equals roughly 111 lb Cover or 203 lb Text, though postcard grades are manufactured as heavy cover boards rather than text sheets.
| Grade | Weight (gsm) | US Cover LB (20 × 26 in) | US Text LB Equiv. (25 × 38 in) | Unlaminated Caliper (mm / in) | Primary Face | Reverse Face |
|---|---|---|---|---|---|---|
| Standard art / C1S / C2S | 300 gsm | ~111 lb Cover | ~203 lb Text | 0.28–0.31 mm (0.0110–0.0122 in) | Coated (C1S/C2S) or uncoated | Uncoated (C1S) or coated (C2S) |
| Heavy art / C1S / C2S | 350 gsm | ~129 lb Cover | ~236 lb Text | 0.34–0.38 mm (0.0134–0.0150 in) | Coated (C1S/C2S) or uncoated | Uncoated (C1S) or coated (C2S) |
| Extra-heavy collector board | 400 gsm | ~148 lb Cover | ~270 lb Text | 0.40–0.44 mm (0.0157–0.0173 in) | Coated (C1S/C2S) or uncoated | Uncoated (C1S) or coated (C2S) |
Double-sided film lamination adds 0.03–0.05 mm (0.0012–0.0020 in) per postcard, raising a 350 gsm board to roughly 0.37–0.43 mm (0.0146–0.0169 in). Single-side film lamination on a C1S front adds roughly half that thickness while keeping the uncoated back open to ink.
Coating Behavior and Reverse-Side Ink Absorption
- C1S (Coated One Side): A clay-coated front holds crisp CMYK halftones and accepts aqueous varnish, UV coating, or film lamination. The uncoated reverse retains open cellulose fibers that absorb ballpoint, rollerball, and gel pen ink without smearing, making C1S the default for mailable postcards.
- C2S (Coated Two Sides): Both faces carry a smooth clay-coated surface that keeps ink on top of the sheet for maximum color saturation and sharp fine detail on both sides. Ballpoint and water-based pens bead or smear on C2S backs unless a matte varnish or uncoated knock-out area is left unvarnished.
- Uncoated Art Board: No clay coating sits on either face, so offset ink penetrates into the fiber matrix. Shadows soften and dot gain increases compared with C2S, while both sides accept handwriting, rubber stamps, and pencil cleanly.
- Film and Varnish Pairings: Anti-scuff matte lamination protects dark-solid artwork from fingernail marks and transit abrasion. Spot UV or spot gloss layers must be excluded from any address or message zone on the reverse face.
Production Steps and Prepress Requirements
Postcard trim dimensions follow the project's assigned format rather than a fixed default, with sheet imposition and grain direction aligned to keep the finished piece flat.
- Prepress File Setup: Supply AI, PDF, or PSD artwork exported as PDF/X-1a or PDF/X-4 at ≥300 DPI with outlined or embedded fonts. Include 3 mm (0.118 in) bleed on every side, keep essential text and logos inside a ≥3 mm (0.118 in) safety margin, and expand the safety margin to ≥4–5 mm (0.157–0.197 in) on bordered backs.
- Ink and Black Separation: Set fine reverse-side text, postal rules, and barcodes in 100% K only. Build large dark backgrounds with rich black (C40–60 M30–40 Y30–40 K100) while keeping total area coverage (TAC) at ≤280%–300% so sheets dry without set-off. Place spot varnish, spot UV, or foil elements on separate spot layers.
- Grain Direction and Offset Printing: Impose postcards with the board grain running parallel to the longer dimension where possible to maximize bending stiffness and minimize curl. Run CMYK plus any spot plates via sheet-fed offset with sufficient drying or IR curing between passes.
- Coating and Lamination: Apply aqueous coating, UV varnish, or thermal film to the coated face(s) after ink cure. Keep the reverse face uncoated or matte-varnished only when pen writeability is required.
- Trimming and Packing: Guillotine-trim stacks to final dimensions with sharp blades to prevent edge chipping on coated faces, then band or box packs by count and weight (tracking pack mass in kg/lb for carton limits).
Sign-Off Criteria
- Caliper and Stiffness: Measured stack or single-card thickness matches the target grade range (for example, 0.34–0.38 mm / 0.0134–0.0150 in for unlaminated 350 gsm stock) with uniform snap across the sheet.
- Writeability Check (C1S / Uncoated): Ballpoint and gel pen marks on the reverse face dry rapidly without beading or smudging when wiped lightly.
- Surface Integrity: Dark CMYK solids and rich black panels show no scuffing, blocking, or ink transfer onto adjacent backs.
- Trim and Registration: Borders stay centered within tolerance, spot coatings align cleanly with underlying CMYK art, and cut edges are free of fiber tear or coating cracks.
Failure Modes
- Smearing on C2S Backs: Writing on a gloss-coated or laminated reverse causes ink to pool and transfer onto other mail or fingers; switch to C1S or leave an uncoated writeable zone.
- Asymmetric Curl on C1S: Heavy single-side thermal film pulls against an unsealed back under humidity swings, bowing the card; balance board weight at 350–400 gsm (0.34–0.44 mm / 0.0134–0.0173 in) or pair a lighter aqueous coating on the front.
- Ink Set-Off and Muddy Shadows: Exceeding TAC 300% on uncoated art board or under-cured C2S causes wet ink to transfer onto the back of the next sheet in the delivery pile.
- Scuffing on Dark Matte Solids: Unprotected matte aqueous varnish marks easily during packing and handling; specify anti-scuff matte film for dark full-bleed designs.
- Edge Cracking on Thick Coated Stock: Dull guillotine knives fracture the clay coating along the cut edge on 350–400 gsm boards, leaving white fiber flakes along dark bleeds.
Parent guide Jigsaw Puzzle and Crowdfunding Paper Extra Materials