Specifications and Tolerances
Postcard board thickness, surface coating, and layout geometry determine how much mechanical deflection occurs under the guillotine knife.
| Parameter | Specification | Notes |
|---|---|---|
| 300 gsm art / blue core | 0.28–0.31 mm (0.011–0.012 in) caliper | Standard baseline for lighter postcards |
| 350 gsm art stock | 0.34–0.38 mm (0.013–0.015 in) caliper | Higher stiffness; requires smaller lifts |
| 400 gsm board | 0.40–0.44 mm (0.016–0.017 in) caliper | Maximum single-ply stiffness; highest blade-draw risk |
| Double-sided film | +0.03–0.05 mm (0.001–0.002 in) per card | Adds slip and thickness; increases stack compression |
| Bleed | 3 mm (0.118 in) per side | Required on all full-bleed and edge-to-edge elements |
| Safety margin (unbordered) | ≥3 mm (0.118 in) inside trim | Keeps text and critical graphics clear of blade variance |
| Safe zone (bordered) | ≥4–5 mm (0.157–0.197 in) inside trim | Absorbs minor trim shift so frames remain visually centered |
| Corner rounding (optional) | R3–R3.5 mm (0.118–0.138 in) | Applied after square guillotine trimming |
- Paper weight basis: Express postcard board weights in gsm alongside US Cover LB (calculated on a 20 × 26 in basis sheet) rather than US Text LB (calculated on a 25 × 38 in basis sheet), so caliper and stiffness expectations remain consistent across mills.
- Prepress file setup: Supply artwork as AI, PDF, or PSD exported to PDF/X-1a or PDF/X-4 at ≥300 DPI in CMYK with separate spot layers. Outline or embed all fonts, set fine text to 100% K, build rich black at C40–60 M30–40 Y30–40 K100, and keep total area coverage (TAC) ≤280%–300%. Anti-scuff matte lamination suits dark bordered artwork by reducing visible clamp and handling marks.
Production Steps
- Imposition and border setup: Position the specified postcard trim format with 3 mm (0.118 in) bleed per side, place all printed borders at ≥4–5 mm (0.157–0.197 in) from the trim line, and include clear corner crop marks and registration targets on the press sheet.
- Lift sizing: Reduce the number of sheets per guillotine lift as caliper increases from 300 gsm (0.28–0.31 mm / 0.011–0.012 in) to 400 gsm (0.40–0.44 mm / 0.016–0.017 in), and reduce lift height further when double-sided film (+0.03–0.05 mm / 0.001–0.002 in per card) creates a slick, compressible stack.
- Clamp-pad installation: Fit a protective false clamp plate or padded clamp shoe to distribute hydraulic clamping force evenly across the lift and prevent metal-on-ink contact.
- Square jogging and clamp dwell: Jog each lift square against the backgauge and side guide. Engage clamp dwell briefly before the knife stroke so trapped air escapes between coated or laminated sheets and the stack locks against the backgauge.
- Trimming: Execute clean single-pass cuts rather than forcing oversized lifts through the blade, keeping knife bevels sharp to shear heavy board without crushing the edge.
Sign-Off Criteria
- Dimensional and border symmetry: Sample cards from the top, middle, and bottom of a trimmed lift match the specified postcard trim dimensions, with opposing border widths appearing visually balanced around the perimeter.
- Edge and surface integrity: Cut edges show no white bleed slivers, no clipped elements inside the ≥3 mm (0.118 in) safety zone (or ≥4–5 mm / 0.157–0.197 in for bordered layouts), and no clamp-bar glossing, scuffing, or fiber bruising on dark rich-black or matte-laminated areas.
- Front-to-back alignment: Backside borders and indicia align cleanly with front artwork within normal sheet registration and guillotine tolerance.
Failure Modes
- Blade draw (top-to-bottom skew): Tall lifts of 350–400 gsm board pull forward under the angled guillotine bevel as the knife descends, leaving bottom sheets slightly wider or shifted compared to top sheets. Reduce lift height and increase clamp dwell before the cut.
- Visually off-center borders: Placing thin frames at ≤3 mm (0.118 in) from the trim line makes minor trim variance immediately noticeable. Keep bordered frames ≥4–5 mm (0.157–0.197 in) inside the trim line or switch to a full-bleed design.
- Clamp bruising and surface burnishing: Unpadded metal clamps crush coated paper fibers or leave shiny marks across dark ink (C40–60 M30–40 Y30–40 K100). Use clamp-pad protection and pair dark bordered designs with anti-scuff matte lamination.
- Edge flaring or film delamination: Dull knives or excessive lift heights on film-laminated 350–400 gsm stock crush the cut edge instead of shearing cleanly, causing white fiber show-through or lifted film edges. Maintain sharp blade schedules and trim smaller lifts.