Specifications

Parameter Specification Notes
Wrap Paper Weight 128–157 gsm Specify in gsm; US Text LB (25 x 38 in / 635 x 965 mm basis sheet) and US Cover LB (20 x 26 in / 508 x 660 mm basis sheet) use different basis sizes and are not interchangeable by pound number.
Paired Greyboard 1.5 / 2 / 2.5 / 3 mm (0.059 / 0.079 / 0.098 / 0.118 in) Thicker boards require clean corner mitering and consistent wrap tension.
Wrap Margin 15–20 mm (0.591–0.787 in) Allowance turned over the greyboard perimeter and anchored on the back face.
Bleed & Safety 3 mm (0.118 in) bleed per side; >= 3 mm (0.118 in) safety Keep critical text and borders at least 3 mm (0.118 in) inside the board edge.
Surface Finish Protective film lamination or varnish Anti-scuff matte film suits dark artwork and high-friction board faces.
File Format & Color AI / PDF / PSD; PDF/X-1a or PDF/X-4 CMYK with separate spot layers; >= 300 DPI; outlined or embedded fonts.
Ink & Black Builds Fine text: 100% K; Rich black: C40–60 M30–40 Y30–40 K100 Keep total area coverage (TAC) <= 280%–300%.

Production Steps

  1. Prepress and Color Separation: Prepare artwork in PDF/X-1a or PDF/X-4 (from AI, PDF, or PSD) at >= 300 DPI with fonts outlined or embedded. Separate spot layers from CMYK, set fine text to 100% K, build large dark areas with rich black (C40–60 M30–40 Y30–40 K100), and cap TAC at <= 280%–300%. Extend background art across the 3 mm (0.118 in) bleed and 15–20 mm (0.591–0.787 in) wrap margin.
  2. Offset Printing: Specialist offset and tabletop manufacturing partners print the 128–157 gsm coated art sheets, maintaining tight registration across full board spreads.
  3. Protective Finishing: Apply protective film lamination or varnish over the printed sheet before board mounting. Use anti-scuff matte film when the face carries dark solids or heavy ink coverage.
  4. Mounting and Hinge Forming: Glue-mount the finished wrap sheet onto 1.5–3 mm (0.059–0.118 in) greyboard, fold the 15–20 mm (0.591–0.787 in) wrap margin tightly around all edges, and press the 180-degree hinge creases so the reinforced film bridges the fold line.

Sign-Off Criteria

  • Basis Weight & Core Match: Wrap paper is 128–157 gsm paired with the specified 1.5, 2, 2.5, or 3 mm (0.059, 0.079, 0.098, or 0.118 in) greyboard.
  • Hinge Integrity: Coated face and protective film or varnish flex through 180-degree hinge creases without white stress lines or ink cracking.
  • Edge & Corner Wrap: The 15–20 mm (0.591–0.787 in) wrap margin adheres flat on the underside with clean, tight corners and no lifting.
  • Print & Color Compliance: Artwork resolves cleanly at >= 300 DPI, fine text prints in 100% K without color halos, rich black falls within C40–60 M30–40 Y30–40 K100, TAC stays <= 280%–300%, and safety elements sit >= 3 mm (0.118 in) inside board edges.

Failure Modes

  • Ink Cracking on 180-Degree Hinges: Unlaminated coated paper or ink builds exceeding 280%–300% TAC fracture along the fold line, exposing white paper fibers under the ink.
  • Surface Scuffing on Dark Artwork: Varnish alone or standard matte finishes show rub marks and shiny streaks across large dark areas during handling; anti-scuff matte film prevents surface abrasion.
  • Edge Lifting and Corner Bunching: A wrap margin narrower than 15 mm (0.591 in) loses grip on 2.5–3 mm (0.098–0.118 in) greyboard edges, while margins wider than 20 mm (0.787 in) or overly stiff sheets bunch at mitered corners.
  • Blurred Fine Text: Setting small type in rich black instead of 100% K introduces multi-plate misregistration and fuzzy edges on coated stock.