Standard single creasing rules work on thin sheet stock because the paper compresses around the fold without excess bulk. On rigid 1.5–3 mm (0.059–0.118 in) greyboard punchboards, a single narrow crease leaves too much core thickness in the hinge, forcing the outer printed paper to stretch over a sharp ridge and split. Selecting between a half-depth cut and a dual-crease channel depends on board caliper, fold angle, and whether the inner core can be exposed:
- Half-depth V-scores / half-cut channels: Cut or mill a partial-depth channel through the greyboard core on the inside of the bend while leaving the outer printed paper intact as the hinge. Use half-depth cuts for crisp 90-degree or 180-degree folds on rigid 1.5 mm (0.059 in), 2 mm (0.079 in), 2.5 mm (0.098 in), and 3 mm (0.118 in) punchboard flaps.
- Dual-crease channels: Place two parallel creasing rules side by side to compress a wider flat hinge across the fold zone. Use dual-crease channels on lighter 1.5 mm (0.059 in) boards or moderate-angle bends where an open V-cut core channel is undesirable.
- Surface finish and ink load: Heavy ink coverage—such as rich black (C40–60 M30–40 Y30–40 K100) near the 280%–300% total area coverage (TAC) limit—shows fiber cracking immediately along a tight fold. Anti-scuff matte lamination or protective film reinforces the outer paper fibers across the hinge.
For how folded flaps interlock with mating tabs and standees, see slot-together punchboard parts.
Specifications and Tooling Parameters
| Parameter | Specification | Notes |
|---|---|---|
| Greyboard core caliper | 1.5 / 2 / 2.5 / 3 mm (0.059 / 0.079 / 0.098 / 0.118 in) | Thicker cores (2.5–3 mm / 0.098–0.118 in) require half-depth V-scores for tight folds |
| Punchboard die gap | 3–4 mm (0.118–0.157 in) | Minimum spacing between adjacent die-cut parts on the sheet |
| Wrap margin | 15–20 mm (0.59–0.79 in) | Allowance for wrapped edges where applicable |
| Bleed | 3 mm (0.118 in) per side | Extends artwork beyond trim edges |
| Safety margin | >= 3 mm (0.118 in) | Keep text and critical graphics clear of trim and fold-channel edges |
| Prepress files & resolution | AI, PDF, or PSD; PDF/X-1a or PDF/X-4; >= 300 DPI | Outlined or embedded fonts; 100% K for fine text |
| Color & ink limits | CMYK + separate spot layers; TAC <= 280%–300% | Separate non-printing spot colors for through-cut, crease, and half-cut paths |
Job-Specific Production Steps
- Separate dieline layers in prepress: Assign distinct non-printing spot colors to perimeter through-cuts, dual-crease rules, and half-depth V-score paths so tooling separates full cuts from partial-depth hinges.
- Protect the fold zone in artwork: Keep fine text and critical graphics at least 3 mm (0.118 in) clear of the fold channel, and hold dark solids within TAC <= 280%–300%.
- Print and laminate the face sheet: Print CMYK at >= 300 DPI and apply anti-scuff matte film when dark artwork crosses a fold line.
- Mount to the greyboard core: Laminate the printed face sheet and backing liner onto the 1.5–3 mm (0.059–0.118 in) greyboard core.
- Score, crease, and die-cut in registration: Form the half-depth V-score or dual-crease channel aligned to the printed fold line, then die-cut the outer part profile across the 3–4 mm (0.118–0.157 in) sheet die gap.
Sign-Off Criteria
- Intact outer wrap: The printed face paper bends cleanly along the fold apex with no fiber tearing, flaking ink, or exposed white paper core.
- Clean hinge closure: Flaps fold to the intended 90-degree or 180-degree angle without spring-back that pulls mating slot-together punchboard parts out of alignment.
- Accurate registration: Fold channels align with the printed graphics and remain outside the 3 mm (0.118 in) safety margin.
- Clean part separation: Parts punch out across the 3–4 mm (0.118–0.157 in) die gap without tearing the scored hinge.
Failure Modes
- Paper cracking and white-line splitting: Caused by running a single narrow crease rule on rigid 1.5–3 mm (0.059–0.118 in) greyboard, or folding heavy unlaminated ink solids without sufficient hinge width.
- Hinge severing (cut-through): Caused by excessive half-cut blade depth cutting into or through the outer printed paper liner instead of stopping at the liner interface.
- Spring-back and flap distortion: Caused by shallow scoring or under-compressed dual creases on 2.5–3 mm (0.098–0.118 in) board, leaving core stiffness that forces the folded flap open.
- Misregistered fold lines: Caused by combining cut and score rules on one spot layer or sheet shift during mounting and die-cutting, placing the fold through graphics inside the 3 mm (0.118 in) safety zone.
Parent guide Slot-Together Paperboard Assemblies