See the finish compatibility overview for how surface coatings interact with other specialty decorations.
Specifications and Compatibility Matrix
Standard offset card runs start at 200 decks (usual production tiers: 200 / 300 / 500 / 1,000+ decks). Card stocks are specified in gsm and fall under US Cover LB (measured on a 20 × 26 in / 508 × 660 mm basis sheet) rather than US Text LB (measured on a 25 × 38 in / 635 × 965 mm basis sheet).
Card Stock, Film Build-Up, and Clearance
| Component / Parameter | Metric (mm) | Imperial (in) | Notes |
|---|---|---|---|
| 300 gsm art / blue-core stock | 0.28–0.31 mm | 0.011–0.012 in | Base caliper before lamination |
| 310 gsm black-core linen stock | 0.30–0.32 mm | 0.012–0.013 in | Textured surface; film bridges linen valleys |
| 330 gsm black-core stock | 0.32–0.34 mm | 0.0126–0.0134 in | Base caliper before lamination |
| 350 gsm art stock | 0.34–0.38 mm | 0.013–0.015 in | Base caliper before lamination |
| 400 gsm card stock | 0.40–0.44 mm | 0.016–0.017 in | Rigid stock; requires sharp die shear |
| PVC card stock | 0.30 mm | 0.012 in | Non-paper core; heat-sensitive under gilding |
| Double-sided film lamination | +0.03–0.05 mm | +0.0012–0.0020 in | Added thickness per finished card |
| Box clearance (width / height) | 1.5–2.5 mm | 0.059–0.098 in | Required around finished deck |
| Box clearance (stack height) | 1.5–3.0 mm | 0.059–0.118 in | Must absorb added film caliper |
Surface Coating vs. Edge Treatment Compatibility
| Surface Finish | Hot-Foil Gilding | Sprayed / Painted Edges | Sanded / Burnished Edges | Primary Physical Constraint |
|---|---|---|---|---|
| Soft-touch lamination | High conflict | Conditional (barrier required) | High conflict | Polyurethane film stretches into edge burrs; clamps glaze the velvet face |
| Anti-scuff matte lamination | Conditional (thin film only) | Compatible (barrier advised) | Conditional (light pass) | Harder topcoat resists clamp scuffing; thick film still resists edge foil |
| Matte offset varnish | Compatible | Compatible | Compatible | No plastic film layer to burr, soften under heat, or peel at the edge |
Prepress and Die-Cut Requirements
- File formats: AI, PDF, or PSD exported as PDF/X-1a or PDF/X-4 with outlined or embedded fonts.
- Color and ink density: CMYK with separate spot layers at ≥300 DPI. Fine text set to 100% K; rich black built as C40–60 M30–40 Y30–40 K100 with Total Area Coverage (TAC) at ≤280%–300%.
- Bleed and safety: 3 mm (0.118 in) bleed per side; ≥3 mm (0.118 in) safety margin, increasing to ≥4–5 mm (0.157–0.197 in) for bordered backs.
- Corner radius: R3–R3.5 mm (0.118–0.138 in). Across custom deck formats, larger or tighter corner radii change how cleanly die blades shear the polyurethane film and how evenly edge foil wraps around the corner.
Job-Specific Production Steps
- Lock finish pairing and stack math before prepress: Confirm whether the deck uses soft-touch lamination with a cold-applied edge color or switches to anti-scuff matte lamination for gilded edges. Add 0.03–0.05 mm (0.0012–0.0020 in) per card to the base stock caliper to verify the finished stack fits within the 1.5–3.0 mm (0.059–0.118 in) box stack-height clearance.
- Print and cure within TAC limits: Run CMYK and spot layers at ≤280%–300% TAC and allow full ink drying before lamination so residual solvents do not outgas and weaken film-to-paper adhesion near the cut edge.
- Apply double-sided lamination: Laminate both faces evenly under controlled tension so the film does not curl the sheet before slitting and die-cutting.
- Die-cut with fresh, sharp tooling: Use sharp cutting rules for the R3–R3.5 mm (0.118–0.138 in) corners and straight edges. Dull blades stretch the elastic polyurethane layer of soft-touch film instead of shearing it cleanly, leaving microscopic burrs along the perimeter.
- Collate with sacrificial protective barriers: Before clamping the deck for edge finishing, place sacrificial guard cards or protective barrier sheets on the top and bottom of the stack. Clamp jaws must never press directly onto the soft-touch face of the finished cards.
- Execute low-abrasion, low-heat edge finishing: Skip aggressive dry sanding on soft-touch decks, as sanding dust embeds into the velvet coating and roughens the perimeter. For painted edges, apply thin, controlled passes with adequate flash-off time between cards so the coating bridges the paper core without pooling onto the film lip.
- De-clamp and inspect edge release: Separate the deck cleanly once the edge treatment cures, ensuring adjacent cards do not tear the soft-touch film at the perimeter.
Sign-Off Criteria
Before approving a production run for pack-out, verify the finished deck against these physical checkpoints:
- Zero clamp glazing on outer cards: Top and bottom cards show uniform matte velvet texture with no shiny compression bands or scuff marks from clamp jaws.
- Burr-free cut edges and corners: Running a finger along the straight edges and R3–R3.5 mm (0.118–0.138 in) corners reveals no raised polyurethane film lips or stringing.
- Continuous edge adhesion: Flexing and riffle-shuffling the deck does not flake edge foil or crack edge paint along the film-to-paper boundary.
- Clean dark-ink faces: Dark solid areas show no white scuff lines, embedded sanding dust, or edge-coating bleed onto the card face.
- Verified box fit: The laminated and edge-finished deck drops into its box or tray within the 1.5–2.5 mm (0.059–0.098 in) width/height and 1.5–3.0 mm (0.059–0.118 in) stack-height clearances.
Concrete Failure Modes
- Clamp Scuffing and Face Glazing: Edge-finishing presses clamp the stacked deck under high pressure to keep edges aligned. Without sacrificial barrier sheets, steel clamp jaws crush the soft-touch polyurethane topcoat on the outer cards, leaving permanent glossy streaks or scuffed patches.
- Polyurethane Film Burrs: Soft-touch film is more elastic than standard OPP matte film. When die-cut with worn blades or lightly sanded before gilding, the film stretches past the paper core and curls into a micro-burr. Edge paint and foil cling to this raised lip rather than the paper core, peeling away during the first shuffle.
- Heat-Induced Film Softening and Weakened Edge Adhesion: Hot-foil gilding transfers heat and pressure along the deck perimeter. Heat softens the soft-touch adhesive and deforms the velvet film edge, causing uneven foil transfer, edge-to-edge blocking (cards sticking together), and premature foil flaking.
- Sanding Dust Contamination and Dark-Artwork Burnishing: Standard edge preparation sands the cut stack smooth before applying pigment or foil. Fine paper and adhesive dust clings electrostatically to soft-touch surfaces, while handling pressure burnishes dark rich-black solids (C40–60 M30–40 Y30–40 K100). Switching to anti-scuff matte lamination eliminates burnishing on dark artwork.
Guides in this section
Parent guide Finish Compatibility
Related guides
- BOPP Lamination and Edge Finishing Compatibility
- Soft-Touch Lamination and Hot Foil Stamping Compatibility
- Soft-Touch Lamination and Spot UV Compatibility
- Full-Bleed Face Decoration and Edge Finishing Compatibility
- Varnish Coatings and Edge Finishing Compatibility
- BOPP Lamination and Hot Foil Stamping Compatibility