Inspection Specifications and Tolerances
Card Deck Press coordinates offset card deck production with specialist manufacturing partners, where paper weight, core opacity, and film thickness determine both single-card caliper and total deck stack height. When comparing US paper specifications, distinguish US Cover LB (based on a 20 × 26 in / 508 × 660 mm basis sheet) from US Text LB (based on a 25 × 38 in / 635 × 965 mm basis sheet), as the same pound rating represents a much heavier caliper in Cover LB than in Text LB.
| Stock Type | Nominal Weight | Uncoated / Base Caliper (mm) | Uncoated / Base Caliper (in) | Primary Inspection Focus |
|---|---|---|---|---|
| Coated art / blue core | 300 gsm | 0.28–0.31 mm | 0.0110–0.0122 in | Core opacity, flat bow, trim centering |
| Black-core linen | 310 gsm | 0.30–0.32 mm | 0.0118–0.0126 in | Linen texture ink lay, edge burr |
| Black core | 330 gsm | 0.32–0.34 mm | 0.0126–0.0134 in | Snap recovery, corner-die cleanliness |
| Coated art stock | 350 gsm | 0.34–0.38 mm | 0.0134–0.0150 in | Stack height fit, surface scuffing |
| Heavy coated art stock | 400 gsm | 0.40–0.44 mm | 0.0157–0.0173 in | Edge cracking on thick film, corner steps |
- Film and coating allowance: Double-sided lamination adds 0.03–0.05 mm (0.0012–0.0020 in) per card. Total deck height is calculated as
(single-card caliper + film allowance) × card count. - Box clearance check: Verify that finished deck dimensions maintain 1.5–2.5 mm (0.059–0.098 in) clearance across width and height, and 1.5–3 mm (0.059–0.118 in) clearance for stack height inside the tuck box or rigid box.
- Trim, bleed, and safety: Production files use 3 mm (0.118 in) bleed per side, ≥3 mm (0.118 in) safety margin for full-bleed art, and ≥4–5 mm (0.157–0.197 in) safety margin for bordered backs. Finished trim-to-border centering must hold within 0.5–1.0 mm (0.020–0.039 in).
- Corner geometry: Standard corner rounding is R3–R3.5 mm (0.118–0.138 in).
- Color and ink limits: Fine text prints in 100% K, and dark backgrounds use rich black (C40–60 M30–40 Y30–40 K100) with total area coverage (TAC) at ≤280%–300%.
Lot Inspection Steps
- Pull samples across sheet positions: Draw decks from the start, middle, and end of the press and cutting run so outer-sheet and inner-sheet positions are represented, especially on 200–1,000+ deck tiers where sheet-to-sheet registration can drift.
- Measure border symmetry and trim centering: On bordered backs, measure opposite margins (left vs. right, top vs. bottom) from the printed border edge to the trimmed edge. Confirm the difference stays within the 0.5–1.0 mm (0.020–0.039 in) centering tolerance and no white bleed edge appears on full-bleed cards.
- Check single-card caliper and deck stack height: Measure individual cards across multiple positions in the deck to confirm they match the specified stock caliper plus 0.03–0.05 mm (0.0012–0.0020 in) when double-sided film is applied. Place the full deck into its matched box to verify 1.5–2.5 mm (0.059–0.098 in) width/height clearance and 1.5–3 mm (0.059–0.118 in) stack height clearance.
- Inspect flat bow and curl: Lay individual cards and full stacks on a flat surface under normal ambient conditions. Check for arched bow along the long or short axis caused by grain direction or unbalanced front-to-back lamination tension.
- Check corner rounding and shuffle-edge burr: Fan the deck and run a finger lightly along all four trimmed edges and R3–R3.5 mm (0.118–0.138 in) corners. Look for stepped corner transitions, fuzzy paper fibers, or raised film lips along the cut edge.
- Evaluate dark-back scratch resistance and edge finishes: Rub two dark-backed cards face-to-back gently under light finger pressure and inspect under angled light for gloss streaks, scuff marks, or ink set-off. On gilded-edge decks, flex the fanned edge to confirm the foil adheres cleanly without peeling against thick lamination.
Sign-Off Criteria
Release the lot only when all sampled decks meet the following physical conditions:
- Centering: Trim-to-border variance is within 0.5–1.0 mm (0.020–0.039 in) on both axes, with no clipped safety-zone elements.
- Edges and corners: R3–R3.5 mm (0.118–0.138 in) corners are symmetrical and smooth, with zero shuffle-edge burr or film delamination along the cut.
- Flatness: Cards sit flat enough to stack cleanly without rocking or springing apart inside the box.
- Surface integrity: Dark rich-black areas show uniform tone without rub marks, smudging, or ink transfer; anti-scuff matte finishes remain matte under light handling.
- Fit: The assembled deck inserts and removes smoothly within the 1.5–2.5 mm (0.059–0.098 in) width/height and 1.5–3 mm (0.059–0.118 in) stack height box clearances.
Concrete Failure Modes and Remedies
- Asymmetric borders on card backs: Caused by guillotine back-gauge drift, sheet skew during die cutting, or designs with less than 4–5 mm (0.157–0.197 in) border safety. Reject affected cutting lifts and re-trim only if remaining margin allows; otherwise reprint with corrected registration or wider borders.
- Shuffle-edge burr and stepped corners: Caused by worn cutting blades, misaligned corner-rounding punches, or heavy 350–400 gsm stock tearing under dull dies. Replace or sharpen cutting dies before continuing the run.
- Dark-back scuffing and ink set-off: Caused by high TAC (>300%) slowing ink cure, standard matte varnish rubbing in transit, or unsealed rich black (C40–60 M30–40 Y30–40 K100). Switch dark-artwork runs to anti-scuff matte lamination or allow full press-sheet curing before cutting.
- Gilded-edge flaking: Caused by thick lamination preventing clean foil adhesion along the deck block edge. Reduce film thickness or adjust edge preparation before gilding.
- Deck bow or curl: Caused by applying film to one side only, uneven moisture absorption between press and bindery, or cutting against optimal paper grain. Balance front-and-back surface coatings and condition sheets before trimming.
Parent guide Card Deck Lot Inspection Checkpoints