Choose a different stock from the card stocks overview when job conditions exceed what a 300 gsm two-ply sheet handles:
- Heavy backlighting or competitive play: Step up to 310 gsm black-core linen (0.30–0.32 mm / 0.012–0.013 in) or 330 gsm black-core stock (0.32–0.34 mm / 0.013–0.013 in) for higher opacity and stiffer snap.
- Rigid non-shuffle reference or display cards: Use 350 gsm art stock (0.34–0.38 mm / 0.013–0.015 in) or 400 gsm stock (0.40–0.44 mm / 0.016–0.017 in) when stiffness matters more than an internal light-blocking core.
- Waterproof or extreme-wear handling: Switch to 0.30 mm (0.012 in) PVC rather than paperboard.
Specifications
| Property | Specification | Notes |
|---|---|---|
| Construction | Two-ply paperboard with pigmented blue adhesive core | Bonds two outer printable plies around a blue barrier |
| Basis weight | 300 gsm (0.30 kg/m² / 0.061 lb/sq ft) | Equivalent to ~111 lb Cover (20 × 26 in / 508 × 660 mm basis sheet) or ~203 lb Text (25 × 38 in / 635 × 965 mm basis sheet); specify Cover LB rather than Text LB |
| Uncoated caliper | 0.28–0.31 mm (0.011–0.012 in) | Measured per single card before film |
| Double-sided film allowance | +0.03–0.05 mm (0.0012–0.0020 in) per card | Brings finished laminated caliper to ~0.31–0.36 mm (0.012–0.014 in) |
| Opacity | Moderate light-blocking | Blocks ambient room light; strong direct backlighting can still cast shadows |
| Corner radius | R3–R3.5 mm (0.118–0.138 in) | Standard rounded playing-card corner profile |
| Bleed & safety | 3 mm (0.118 in) bleed per side; ≥3 mm (0.118 in) safety | Increase safety to ≥4–5 mm (0.157–0.197 in) for bordered card backs |
| Prepress file setup | AI, PDF, or PSD exported as PDF/X-1a or PDF/X-4 | CMYK with separate spot layers, ≥300 DPI, outlined or embedded fonts |
| Ink & black build | 100% K for fine text; rich black C40–60 M30–40 Y30–40 K100 | Keep Total Area Coverage (TAC) ≤280%–300% |
| Box clearance | 1.5–2.5 mm (0.059–0.098 in) width/height; 1.5–3 mm (0.059–0.118 in) stack height | Size packaging from final coated stack height, not uncoated caliper |
Production Steps
- Two-ply lamination and conditioning: Specialist paper mills bond two outer paper plies with a pigmented blue adhesive layer. Sheets are conditioned to equalize moisture across both plies before entering the pressroom.
- Offset printing: Print CMYK and any separate spot layers onto the outer plies while holding TAC ≤280%–300%. Keeping ink density balanced between face and back prevents one ply from expanding faster than the other.
- Coating or film lamination: Apply protective varnish or double-sided film (+0.03–0.05 mm / 0.0012–0.0020 in per card). Use anti-scuff matte film on dark artwork to reduce visible rub marks; avoid thick lamination if the deck also specifies gilded edges, as thick film can conflict with edge gilding.
- Slitting, corner rounding, and collating: Cut sheets to the job's assigned trim dimensions, round corners to R3–R3.5 mm (0.118–0.138 in) with sharp dies, and collate decks into boxes sized with 1.5–2.5 mm (0.059–0.098 in) width/height clearance and 1.5–3 mm (0.059–0.118 in) stack-height clearance.
Sign-Off Criteria
- Caliper and stack height: A 10-card or full-deck stack averages 0.28–0.31 mm (0.011–0.012 in) per uncoated card, or 0.31–0.36 mm (0.012–0.014 in) with double-sided film, and slides into its box with 1.5–3 mm (0.059–0.118 in) stack clearance.
- Casual light blocking: Under normal ambient room lighting, dark face graphics do not show through the card back.
- Flatness and snap: Cards lie flat on a level surface without edge cupping, return cleanly after a gentle flex, and show no ply separation along cut edges or R3–R3.5 mm (0.118–0.138 in) corners.
- Print and border registration: Fine text renders sharply in 100% K, rich black solids are free of mottling or set-off, and bordered backs remain visually centered within the ≥4–5 mm (0.157–0.197 in) safety margin.
Failure Modes
- Two-ply moisture curl: Because blue-core stock consists of two paper plies joined by adhesive, unequal moisture uptake—from heavy ink coverage on one side, unbalanced one-sided coating, or humid storage—causes cupping or bowing. Keep TAC ≤280%–300%, coat both sides evenly, and condition sheets before cutting.
- Edge or corner delamination: Dull cutting dies, uncured adhesive, or excessive shear during R3–R3.5 mm (0.118–0.138 in) corner rounding can split the two plies along the blue adhesive line. Maintain sharp tooling and verify ply bond strength before full-run die-cutting.
- Backlit show-through: Blue-core adhesive provides moderate opacity rather than total light blocking. High-contrast black-and-white card faces held against a bright direct light source can still shadow through; move to 310–330 gsm black-core stock when full opacity is required.
- Creasing under heavy shuffle stress: At 300 gsm (0.28–0.31 mm / 0.011–0.012 in), repeated sharp bending fatigues the fibers sooner than thicker black-core boards, softening snap over time.
- Tight box fit: Calculating box depth from uncoated caliper instead of adding 0.03–0.05 mm (0.0012–0.0020 in) per card for double-sided film eliminates the 1.5–3 mm (0.059–0.118 in) stack clearance across a full deck, causing jammed cards or bowed box panels.
Parent guide Card Stocks and Paper Core Construction